各种永磁材料的性能和饱和磁化场
各种永磁材料的性能和饱和磁化场 | ||||||||
种类 | 牌号 | 剩磁Br | 矫顽力Hc | 最大磁能积 (BH)max | 相对回复磁 导率μrec | 磁温度系数 αB | 居里点 Tc | 饱和磁化场⑤ |
T | kA/m | kJ/m3 |
| %℃-1 | ℃ | kA/m | ||
铝 镍 钴 合 金 ① | LN10﹡ | 0.60 | 40 | 9.6 | 4.5~5.5 | -0.022 | 760 | 200 |
LNG12 | 0.70 | 40 | 12 | 6.0~7.0 |
| 810 | 240 | |
LNG34 | 1.20 | 44 | 34 | 4.0~5.0 |
|
| 240 | |
LNG37 | 1.20 | 48 | 37 | 3.0~4.5 | -0.016 | 890 | 240 | |
LNGT28 | 1.00 | 58 | 28 | 3.5~5.5 |
| 860 |
| |
LNGT38 | 0.80 | 110 | 38 | 1.5~2.5 | -0.020 | 850 | 400 | |
LNGT36J | 0.70 | 140 | 36 | 1.5~2.5 |
|
|
| |
LNG44 | 1.25 | 52 | 44 | 2.5~4.0 | -0.016 |
| 240 | |
LNG52 | 1.30 | 56 | 52 | 1.5~3.0 | -0.016 | 890 | 240 | |
LNGT60 | 0.90 | 110 | 60 | 1.5~2.5 | -0.020~-0.025 | 850 | 400 | |
LNGT72 | 1.05 | 112 | 72 | 1.5~2.5 | -0.020~-0.025 | 850 | 400 | |
FLN8﹡ | 0.52 | 40 | 8 | 4.5~5.5 |
| 760 | 200 | |
FLNG28 | 1.05 | 46 | 28 | 4.0~5.0 |
| 890 | 240 | |
FLNG34 | 1.12 | 47 | 34 | 3.0~4.5 |
| 890 | 240 | |
FLNGT31 | 0.76 | 107 | 31 | 2.0~4.0 |
| 850 | 400 | |
FLNGT33J | 0.65 | 136 | 33 | 1.5~3.5 |
|
|
| |
铁 氧 体 永 磁 材 料 ② | Y10T﹡ | ≥0.20 | 128~160 | 6.4~9.6 | 1.05~1.3 | -0.18~-0.20 | 450 | 800 |
Y15 | 0.28~0.36 | 128~192 | 14.3~17.5 | 450~460 | ||||
Y20 | 0.32~0.38 | 128~192 | 18.3~21.5 | 450~460 | ||||
Y25 | 0.35~0.39 | 152~208 | 22.3~25.5 | 450~460 | ||||
Y30 | 0.38~0.42 | 160~216 | 26.3~29.5 | 450~460 | ||||
Y35 | 0.40~0.44 | 176~224 | 30.3~33.4 | 450~460 | ||||
Y16H | ≥0.31 | 232~248 | ≥17.6 | 460 | ||||
Y20H | ≥0.34 | 248~264 | ≥21.5 | 460 | ||||
Y25BH | 0.36~0.39 | 176~216 | 23.9~27.1 | 460 | ||||
Y30BH | 0.38~0.40 | 224~240 | 27.1~30.3 | 460 | ||||
稀 土 钴 永 磁 材 料 ③ | XG80/36 | 0.60 | 310 | 64~68 | 1.10 | -0.09 | 450~500 | 1600 |
XG96/40 | 0.70 | 350 | 88~104 | 1.10 | -0.09 | 450~500 | 1600 | |
XG112/96 | 0.73 | 520 | 104~120 | 1.05~1.10 | -0.05 | 700~750 | 2400 | |
XG128/120 | 0.78 | 560 | 120~140 | 1.05~1.10 | -0.05 | 700~750 | 2400 | |
XG144/120 | 0.84 | 600 | 140~150 | 1.05~1.10 | -0.05 | 700~750 | 2400 | |
XG144/56 | 0.84 | 520 | 140~150 | 1.00~1.05 | -0.05 | 700~750 | 2400 | |
XG160/120 | 0.88 | 640 | 150~184 | 1.05~1.10 | -0.05 | 700~750 | 3200 | |
XG196/96 | 0.96 | 690 | 184~200 | 1.05~1.10 | -0.05 | 700~750 | 3200 | |
XG169/42 | 096 | 400 | 184~200 | 1.00~1.05 | -0.03 | 800~850 | 1600 | |
XG208/44 | 1.00 | 420 | 200~220 | 1.00~1.05 | -0.03 | 800~850 | 1600 | |
XG240/46 | 1.06 | 440 | 220~250 | 1.00~1.05 | -0.03 | 800~850 | 1600 | |
可塑性永 磁材料④ | 2J83 | 1.05 | 48 | 24~32 |
|
|
|
|
2J84 | 1.20 | 52 | 32~40 |
|
|
|
| |
2J85 | 1.30 | 44 | 40~48 |
|
|
|
| |
注:﹡表示各向同性,未加﹡者为各向异性。 ①摘自GB4754—84《铝镍钴永磁(硬磁)合金技术条件》。②摘自SJ285—77《永磁铁氧体材料》。③摘自《稀土钴永磁材料标准草案》。④摘自《变形铁铬钴永磁合金标准草案》。⑤摘自GB3218—82《永磁(硬磁)材料磁性试验方法》。 | ||||||||